版權(quán)說明:本文檔由用戶提供并上傳,收益歸屬內(nèi)容提供方,若內(nèi)容存在侵權(quán),請進行舉報或認領(lǐng)
文檔簡介
TestReport
Client:Address:
ShanghaiHanshiMoldingShapeCo.,Ltd.
No.355,YouDongRoad,Shanghai,P.RChina
DUNS: —
TestedSample: ASSYFRONTBEAMPartNumber:55005311
SampleDescription: Model:C30
Materialandgrade:P7-GF45-0790-BK711
ReceivingDate: 2015-03-12 EvaluationType:—
TechnicalSpecification:GMW14650-2013
TestItems:
TestResults:
DimensionalStability
ResistancetoTemperature-HumidityCycle(DimensionalStability)
ResistancetoHigh-HumidityEnvironment
ImpactResistance
Accordingtoclient’srequirements,thetesthasbeenconductedonreceivedsamples.Refertopage2fordetailsofresults.
Editedby:ZhangWeiqi
Checkedby:NingWentao
Approvedby:
Signature:
Signature:
Signature:
Dateofissue:
TestSummary
SectionNo.
ClauseNo.
TestItem
Ref.Standard
Evaluation
Section001
Accordingtoclient’s
requirements
DimensionalStability
Accordingtoclient’s
requirements
Pass
Section002
GMW14650-2013
§4.3
ResistancetoTemperature-HumidityCycle(Dimensional
Stability)
GMW14650-2013
—
Section003
GMW14650-2013
§4.4
Resistanceto
High-HumidityEnvironment
GMW14729-2010
Pass
Section004
GMW14650-2013
§4.9
ImpactResistance
GMW14093-2013
Pass
D15009701
SamplePhotos
Section001DimensionalStability
Ref.
Standard
Client`srequirement
DateofTest
2015-03-25~2015-03-26
Tested
SampleID.
D150097010102
TestConditions
A:After8hunder110℃,theproductcontourdeformationcomparedwiththeoriginal,parts,evaluation:heightofZ5comparedwiththeinitialstateofnomorethan2mm;
B:Toputproductsatroomtemperature(23±3℃),fromAstateslowlycooledtoBstatemeasurement,evaluation:heightofZ5comparedwiththeinitialstateislessthan1mm;
A:After8hunder-40℃,theproductcontourdeformationcomparedwiththeoriginal,parts,evaluation:heightofZ5comparedwiththeinitialstateofnomorethan2mm;
B:Toputproductsatroomtemperature(23±3℃),fromAstateslowlycooledtoBstate
measurement,evaluation:heightofZ5comparedwiththeinitialstateislessthan1mm.
TestInstruments
No.
Name
Type
Number
Calibration
ValidDate
1
Highandlowtemperature
testchamber
SDJ41FD
EQ-0032
2015.09.02
Test
Requirement
SeeTestConditions(Accordingtothecustomer’srequirements)
TestResults
Sampl
No.
Condition
Change(mm)
Verdict
Z1
Z6
Z7
Z8
Z9
Z10
1#
Afterhightemp
0.07
0.04
0.66
0.21
0.47
0.66
P
Roomtemp
0.03
0.01
0.55
0.20
0.25
0.50
P
Afterlowtemp
0.58
0.34
0.74
0.41
0.45
0.40
P
Roomtemp
0.12
0.40
0.50
0.30
0.22
0.31
P
2#
Afterhightemp
0.11
0.18
0.54
0.58
0.40
0.54
P
Roomtemp
0.36
0.16
0.48
0.41
0.31
0.15
P
Afterlowtemp
0.42
0.33
0.67
0.02
0.44
0.24
P
Roomtemp
0.35
0.20
0.45
0.40
0.20
0.15
P
3#
Afterhightemp
0.08
0.07
0.74
0.14
0.45
0.75
P
Roomtemp
0.05
0.04
0.31
0.05
0.22
0.55
P
Afterlowtemp
0.12
0.02
0.41
0.20
0.35
0.45
P
Roomtemp
0.10
0.00
0.32
0.18
0.24
0.15
P
Test
Conclusions
Pass
Remark
P:Pass;F:Fail;“—”:NotApplicable
TestPictures
Testing
Testing
Section002ResistancetoTemperature-HumidityCycle(DimensionalStability)
Ref.
Standard
GMW14650-2013
DateofTest
2015-03-25~2015-04-09
Tested
SampleID.
D150097010401
Sample
Quantity
3pcs
TestConditions
Thiscycleshallbecarriedouttwotimeswithoutinterruption:
Cycle:17±0.5h,-30±3℃→72±1hat85±3℃→24±1h,38±2℃,100%RH→7h±0.5h,
-30±3℃→24±1h,38±2℃,100%RH→24±1h,22±3℃
Checktheappearanceandthedimensionscomparedwiththeoriginalparts.
TestInstruments
No.
Name
Type
Number
Calibration
ValidDate
1
Highandlow
temperaturetestchamber
SDJ610A
EQ-0069
2015.12.14
TestRequirement
Appearance:Testpiecesshallshownocracking,crazing,appreciablecolorchanges,discoloration,cloudiness,blistering,objectionableshrinkage,anddeformation,lossofadhesiontothesubstratebetweenlayersofthecompositeorotherchangesdetrimentalto
serviceability.
TestResults
SampleNo.
Result
Verdict
Appearance
Dimension
1#
Shownocracking,crazing,appreciablecolor
changes,discoloration,cloudiness,blistering,objectionableshrinkage,anddeformation,
Seethenextpage
—
2#
Shownocracking,crazing,appreciablecolorchanges,discoloration,cloudiness,blistering,
objectionableshrinkage,anddeformation,
—
3#
Shownocracking,crazing,appreciablecolor
changes,discoloration,cloudiness,blistering,objectionableshrinkage,anddeformation,
—
Test
Conclusions
—
Remark
P:Pass;F:Fail;“—”:NotApplicable
SampleNo.
Condition
Result(mm)
1#
Change
Z1
Z6
Z7
Z8
Z9
Z10
-0.11
-0.41
-0.05
-1.31
-1.46
-0.86
2#
Z1
Z6
Z7
Z8
Z9
Z10
-0.57
-1.47
-2.03
-1.41
-1.32
2.25
3#
Z1
Z6
Z7
Z8
Z9
Z10
-1.10
-1.97
-2.65
-1.32
-1.32
-1.87
Section002ResistancetoTemperature-HumidityCycle(DimensionalStability)
TestPictures
Pre-test1#
Pre-test1#
Pre-test2#
Pre-test2#
Pre-test3#
Pre-test3#
Testing
Post-test1#
Post-test1#
Post-test2#
Post-test2#
Post-test3#
Post-test3#
Section003ResistancetoHigh-HumidityEnvironment
Ref.
Standard
GMW14729-2010
DateofTest
2015-03-20~2015-03-27
Tested
SampleID.
D150097010104
TestConditions
Measurethedimensionsoftestpiecesbeforetest;
Placetestpiecesat(40±3)℃,~100%RHfor(168±2)hand(22±3)℃,(50±5)%RHfor24h;
Evaluatethesurfacevisuallyandmeasurethedimensionsoftestpiecesaftertest.
TestInstruments
No.
Name
Type
Number
Calibration
ValidDate
1
Highandlowtemperature
testchamber
SDJ610A
EQ-0069
2015.12.14
TestRequirement
Testpiecesshallshownosignificantsurfacechanges,particularlychangesincolororgloss,orotherchangesdetrimentaltoserviceability.Thedimensionsshouldbeno
significantchanges.
TestResults
Seethenextpage.
Test
Conclusions
Pass
Remark
P:Pass;F:Fail;“—”:NotApplicable
SampleNo.
Result
Verdict
Appearance
1#
Shownosignificantsurfacechanges
P
2#
Shownosignificantsurfacechanges
P
3#
Shownosignificantsurfacechanges
P
SampleNo.
Change(mm)
Z1
Z6
Z7
Z8
Z9
Z10
1#
0.24
0.77
0.04
0.41
0.22
0.07
2#
0.15
0.61
0.23
0.11
0.06
0.14
3#
0.04
0.54
0.14
0.05
0.21
0.91
Section003ResistancetoHigh-HumidityEnvironment
TestPictures
Testing
Testing
1#Pre-test
1#Post-test
2#Pre-test
2#Post-test
3#Pre-test
3#Post-test
Section004ImpactResistance
Ref.
Standard
GMW14093-2013
DateofTest
2015-04-13~2015-04-14
Tested
SampleID.
D150097010501
TestConditions
Testintheas-receivedcondition,afterheatagingandaftertemperaturecycling;
Conditioning:(22±3)°C&(50±5)%RHfor24h;
Freezertemperature:-30°C;Freezingtime:4h;Impactenergy:5J.
TestInstruments
No.
Name
Type
Number
Calibration
ValidDate
1
Lowtemperature
freezingfreezer
DW-FW251
EQ-0101
2015.07.21
2
Fallingballimpact
tester
LQ-001
YQ-0069
2015.12.15
Test
Requirement
Nocracksorbreakage.
TestResults
SampleNo.
Result
Verdict
As-received
1#
Nocracksorbreakage
P
2#
Nocracksorbreakage
P
3#
Nocracksorbreakage
P
Afterheataging
4#
Nocracksorbreakage
P
5#
Nocracksorbreakage
P
6#
Nocracksorbreakage
P
After
temperaturecycling
7#
Nocracksorbreakage
P
8#
Nocracksorbreakage
P
9#
Nocracksorbreakage
P
Test
Conclusions
Pass
Remark
P:Pass;F:Fail;“—”:Notapplicable;
Wedirectlyusedthesamplesthathadbeentreatedintheagingtestandtemperaturecyclingtesttoperformimpacttest.
Section004ImpactResistance
TestPictures
Testing
Testi
溫馨提示
- 1. 本站所有資源如無特殊說明,都需要本地電腦安裝OFFICE2007和PDF閱讀器。圖紙軟件為CAD,CAXA,PROE,UG,SolidWorks等.壓縮文件請下載最新的WinRAR軟件解壓。
- 2. 本站的文檔不包含任何第三方提供的附件圖紙等,如果需要附件,請聯(lián)系上傳者。文件的所有權(quán)益歸上傳用戶所有。
- 3. 本站RAR壓縮包中若帶圖紙,網(wǎng)頁內(nèi)容里面會有圖紙預(yù)覽,若沒有圖紙預(yù)覽就沒有圖紙。
- 4. 未經(jīng)權(quán)益所有人同意不得將文件中的內(nèi)容挪作商業(yè)或盈利用途。
- 5. 人人文庫網(wǎng)僅提供信息存儲空間,僅對用戶上傳內(nèi)容的表現(xiàn)方式做保護處理,對用戶上傳分享的文檔內(nèi)容本身不做任何修改或編輯,并不能對任何下載內(nèi)容負責(zé)。
- 6. 下載文件中如有侵權(quán)或不適當(dāng)內(nèi)容,請與我們聯(lián)系,我們立即糾正。
- 7. 本站不保證下載資源的準(zhǔn)確性、安全性和完整性, 同時也不承擔(dān)用戶因使用這些下載資源對自己和他人造成任何形式的傷害或損失。
最新文檔
- 2025年寧夏藝術(shù)職業(yè)學(xué)院高職單招職業(yè)適應(yīng)性測試歷年(2019-2024年)真題考點試卷含答案解析
- 2025年寧夏建設(shè)職業(yè)技術(shù)學(xué)院高職單招職業(yè)適應(yīng)性測試歷年(2019-2024年)真題考點試卷含答案解析
- 花卉網(wǎng)店創(chuàng)業(yè)路演
- 年終盛典:總結(jié)與展望
- 血管內(nèi)超聲護理配合
- 荷葉古典文化教育知識
- 2025年福建省德化一中、永安一中、漳平一中高三1月模擬考試物理試題含解析
- 云南省大理市2025年高三4月考生物試題含解析
- 學(xué)校特色課程介紹
- 重慶三峽學(xué)院《食品無損檢測》2023-2024學(xué)年第二學(xué)期期末試卷
- 展覽會議展前展中展后服務(wù)方案(技術(shù)方案)
- 2025年山東淄博高三一模高考數(shù)學(xué)試卷試題(含答案詳解)
- 建筑垃圾處理工地安全事故應(yīng)急預(yù)案
- 2025年湖北省恩施市司法局司法輔助人員招聘9人歷年高頻重點提升(共500題)附帶答案詳解
- 2024-2030年中國玄武巖纖維工業(yè)行業(yè)現(xiàn)狀調(diào)研及投資戰(zhàn)略研究報告
- 項目部組織機構(gòu)和管理體系范文
- 自然辯證法論述題146題帶答案(可打印版)
- 2024-2030年中國鹽差能行業(yè)面臨的困境分析及投資規(guī)模研究報告
- 七年級語文上冊語文必背【古詩詞與文言文】
- 小學(xué)生火星天問一號祝融車分享
- 全過程造價咨詢項目保密及廉政執(zhí)業(yè)措施
評論
0/150
提交評論